A-286 Stainless Steel Sheet & Coil
.
Iron-Base Superalloy
Type A286 (UNS Designation S66286)
Physical Properties
| Solution Treated | Solution Treated and Aged |
| Density |
0.286 lb./in3 (7.92 g/cm3) |
0.287 lb./in3 (7.94 g/cm3) |
| Specific Gravity |
7.92 |
7.94 |
| Melting Range |
2500 - 2600 °F |
1370 - 1430 °C |
| Magnetic Permeability |
1.010 |
1.007 |
Thermal Conductivity
| Temperature Range |
Linear Coefficients of Thermal Expansion · 10-6 |
| °C |
°F |
/°C |
/°F |
| 21 - 93 | 70 - 200 | 16.5 | 9.17 |
| 21 - 204 | 70 - 400 | 16.8 | 9.35 |
| 21 - 316 | 70 - 600 | 17.0 | 9.47 |
| 21 - 427 | 70 - 800 | 17.4 | 9.64 |
| 21 - 538 | 70 - 1000 | 17.6 | 9.78 |
| 21 - 649 | 70 - 1200 | 17.8 | 9.88 |
| 21 - 760 | 70 - 1400 | 18.6 | 10.32 |
Thermal Conductivity
| Temperature Range |
Coefficients |
| °C |
°F |
W/m·K |
Btu/(hr/ft²/in/°F) |
| 150 | 302 | 15.1 | 8.7 |
| 300 | 572 | 17.8 | 10.3 |
| 500 | 932 | 21.8 | 12.6 |
| 600 | 1112 | 23.9 | 13.8 |
Specific Heat
420 Joules/kg °K (Btu/lb/°F)
Electrical Resistivity
| Temperature |
microhm-cm |
| °C |
°F |
| 25 | 77 | 91.0 |
| 540 | 1004 | 115.6 |
| 650 | 1202 | 118.8 |
| 730 | 1346 | 120.1 |
| 815 | 1499 | 122.4 |
Back to A-286 Alloy
Instant Online Quote (Sheet)
Request for Quote (Coil)
We stock only prime metals and alloys that are certified to AMS, MILS and ASTM specifications. Materials are ordered not by just gauge, but to precise decimal thickness.